Author: Subject:  Metal Shrinking
Memberbevoracing
A.k.a.: Tony Beven
Officially Full-On Dubber
***


Avatar


Posts: 326
Threads: 36
Registered: January 18th, 2009
Member Is Offline

Location: Mount Pleasant SA
Theme: UltimaBB Vintage
Mood: Leaning against the shed wall !.

posted on May 1st, 2011 at 08:46 PM
Metal Shrinking


The trouble with Country Buggy panels is that they were (almost) flat, and flat is a very hard thing to get them back to. Any kind of dent at all represents a “stretch” of the metal. Country Buggies are utilitarian so they’ve all been climbed on and had materials thrown in them. Mine, KO813 only has a few straight pieces of metal, and most of them have holes that need welding up.
This weekend I’ve been experimenting with the alchemy of metal shrinking. I followed the instructions from here:- http://www.carrepair-1950.com/shrinking-sheet-metal.htm
It works great. After beating the dents out you will always end up with a bulge, and using this technique it can be disappeared. I used an Oxy torch but I expect a carbon arc attachment on a welder would do, anything that will make it red hot.
Now, this bloke talks about getting it so straight you don’t have to use any filler. These panel beater blokes know some secret squirrel trick that I don’t know, that’s for sure. Anyway, hope it helps someone out.
Cheers
Tony




Country Buggy King & Link Pin Overhauls, Type 1 & 2 King Pins, General Machining.
http://forums.aussieveedubbers.com/viewtopic.php?tid=74138 
My car is KO813
MemberHappyDaze
A.k.a.: Greg Mackie
Son of Jim - Creator of Good
Superannuated
******


Avatar


Posts: 2887
Threads: 141
Registered: June 13th, 2009
Member Is Offline

Location: Southern Highlands NSW
Theme: UltimaBB Pro Blue ( Default )
Mood: Happy enough

posted on May 1st, 2011 at 09:13 PM



May I just add that using a wet rag to cool the hot metal down, after the 'shrink' is completed, will help. It will also speed up the process. Oxy is best to heat the 'spot', using a small tip.



I'd rather wear a Beetle out by racing it than by polishing it!
Super Administratorhelbus
A.k.a.: Pete S
Super Administrator
Mad fabricator, paint and body
*********

Rank Avatar

Avatar


Posts: 7386
Threads: 312
Registered: September 1st, 2002
Member Is Offline

Location: In the garage chopping cars into bits
Theme: UltimaBB Pro Blue
Mood: In the thinking chair

posted on May 1st, 2011 at 09:19 PM



There is no secret. It requires skill and patience. I have been doing it for 20 years, and I consider myself very skilled in metal shrinking, and still it can take many hours to get a flat panel 'tight'. Eventually you can get a flat panle perfect requiring no filler, however the customer often does not want 20 hours labour cost repairing something that can be made in 10 hours.



MemberFlintstones
Custom Title Time!
*****


Avatar


Posts: 1077
Threads: 69
Registered: August 27th, 2002
Member Is Offline

Location: Sydney
Theme: UltimaBB Psyche Blue

posted on May 1st, 2011 at 11:47 PM



another technique I found works great is to use a shrinking disk.
You can cover a lot of area very quickly where as with an oxy torch, you can only work one spot (usually the size of a 5 or 10 cent coin) at a time.
Do a search on you tube and you'll find some examples.

Cheers
D
Super Administratorhelbus
A.k.a.: Pete S
Super Administrator
Mad fabricator, paint and body
*********

Rank Avatar

Avatar


Posts: 7386
Threads: 312
Registered: September 1st, 2002
Member Is Offline

Location: In the garage chopping cars into bits
Theme: UltimaBB Pro Blue
Mood: In the thinking chair

posted on May 2nd, 2011 at 12:03 AM



You will see on the you tube that the shrinking disc is all on panels with a round curve shape.

A flat flat panel has to be shrunk using oxy torch. Very tricky and takes a lot of time.

If you have lots of shaping, shrinking and welding to do, the oxy is the primary welding/ heating tool. You just need to get a bit of experience, and you will find you can make anything. The prototype 1 of a kind cars I work on are all made from flat sheet using oxy.




Memberbevoracing
A.k.a.: Tony Beven
Officially Full-On Dubber
***


Avatar


Posts: 326
Threads: 36
Registered: January 18th, 2009
Member Is Offline

Location: Mount Pleasant SA
Theme: UltimaBB Vintage
Mood: Leaning against the shed wall !.

posted on May 2nd, 2011 at 03:55 PM



Ahh, there’s the secret, 20 years of experience. I’ll keep at it Helbus, one day perhaps.

You are quite right Mr Daze, I was using a wet rag. There was another article on the internet somewhere by a very experienced panel beater but I can’t find it now. He mentioned all your points exactly.

There is quite a lot of conflicting info on the net, as with all subjects. Some like shrinking discs but say they are hard to find, some talk about using a worn out sanding disc, sounds a bit scary. Others don’t like any discs, just Oxy etc. Some like letting it cool on it’s own, some use compressed air, some like water. Some say it makes no difference, some say it does. Interesting subject.




Country Buggy King & Link Pin Overhauls, Type 1 & 2 King Pins, General Machining.
http://forums.aussieveedubbers.com/viewtopic.php?tid=74138 
My car is KO813


  Go To Top


Powered by GaiaBB, © 2011 The GaiaBB Group
(C) 2001-2024 Aussieveedubbers

[ Queries: 40 ] [ PHP: 30.9% - SQL: 69.1% ]